Sn-based babbitt metal - Chemical etching

Material Name: Sn-based babbitt metal
Recipe No.: 11067
Primary Chemical Element in Material: Sn
Sample Type: Bulk
Uses: General microstructure
Etchant Name: None
Type (Macro/Micro): Micro
Etching Method: Chemical
Etchant (Electrolyte) Composition: 95 ml distilled water, 2 ml HCl, 5 ml HNO3.
Procedure (Condition): Immerse sample up to 5 min.
Note: No data
Reference: Vander Voort, Metallography Principles and Practice, McGraw-Hill, Inc., 1986, p. 690.