19MnVS6 Steel

Steel name: 19MnVS6
Diagram No.: 1430
EN designation: 19MnVS6
r> Chemical composition in weight %: 0.17-0.20% C, 0.30-0.45% Si, 1.45-1.60% Mn, max. 0.030% P, 0.020-0.035% S, 0.20-0.30% Cr, max. 0.30% Ni, 0.08-0.12% V
Steel group: Micro Alloy steels
Applications: Suitable for case carburizing or nitriding.
Comment: Jominy hardenability according to ASTM A255. The graph shows the average values, standard deviation (error bars) and minimum/maximum values for steel.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: QT: 900-950 C/water, as-carburized: 850-910 C/oil, tempering: QT: 500 - 650 C, as-carburized: 150-200 C.

Hardenability Diagram

Price: 20.00 US $
Buy Online Hardenability Diagram

Other Steel Data links:
Carbides in Steel
CCT & TTT Diagrams of Steels
Etchants Database
Hardenability Calculating Service
Macro Defects in Steel
Non-Metallic Inclusions in Steel
Tempering Diagrams of Steels

Disclaimer: The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other purposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2017 by Steel Data. All Rights Reserved.