1.7131 Steel

Steel name: 1.7131
Steel name of producers:
16MnCr5 DIN EN 10084:2008-06 Germany
16MnCr5 DIN EN 10132-2:2000-05 Germany
16MnCr5 DIN EN 10263-3:2002-02 Germany
16MnCr5 DIN EN 10297-1:2003-06 Germany
16MnCr5 Stahl Eisen List: 2004 Germany
16MnCr5 AFNOR EN 10084:1999-03 France
16MnCr5 UNE EN 10084:1998 Spain
16MnCr5 Dillinger Hüttenwerke Germany
16MnCr5 Dirostahl Germany
EC80 Eschmann-Stahl Germany
16MnCr5 HKM Krupp Mannesmann Germany
16MnCr5 Hover&Sohn Germany
16MnCr5 Platestahl Germany
16MnCr5 Saarstahl Germany
16MnCr5 Thyssen Edelstahl Service GmbH Germany
TEW16MnCr5 Thyssen Edelstahl Service GmbH Germany
16MnCr5 Zapp Germany
16MnCr5 DIN EN 10084:1998-06 Germany
16MnCr5 DIN 1652-3:1990-11 Germany
16MnCr5 DIN 1654-3:1989-10 Germany
16MC5 AFNOR EN 10084:1994 France
16MnCr5 AFNOR EN 10084:1994 France
16MnCr5 DDR-TGL Germany
E410 Bohler Uddeholm Austria
ECM Deutsche Edelstahlwerke (Witten-Krefeld) Germany
1.7131 Hoverstahl Germany
16MnCr5 Krupp Germany
EC80 Röchling Germany
E410 Bohler Uddeholm Germany
Diagram No.: 4626
Type of diagram: CCT
Mat. No. (Wr. Nr.) designation: 1.7131
Chemical composition in weight %: 0.16% C, 0.22% Si, 1.12% Mn, 0.030% P, 0.008% S, 0.99% Cr, 0.02% Mo, 0.12% Ni, 0.010% V, 0.015% Al
Steel group: Structural steels
Note: Alloy special structural steels. Austenitizing temperature: 830oC, time: 15 min, carburizing: about 0.9% C.
Reference: Not shown in this demo version.

Transformation Diagram

Price: 30.00 US $
Buy Online Transformation Diagram

Other Steel Data links
Carbides in Steel
Etchants Database
Hardenability Diagrams of Steels
Macro Defects in Steel
Non-Metallic Inclusions in Steel
Tempering Diagrams of Steels
CCT and TTT Diagram Calculating Service

Disclaimer: The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2019 by Steel Data. All Rights Reserved.