InSb - Dislocation etching

Material Name: InSb
Recipe No.: 10189
Primary Chemical Element in Material: In
Sample Type: Bulk
Uses: Etching
Etchant Name: None
Type (Macro/Micro): Micro
Etching Method: Dislocation etching
Etchant (Electrolyte) Composition: HF and HNO3 equal parts.
Note: (110)
Procedure (Condition):  Eth for 2-5 s. Venables and Broudy.
Reference: Vander Voort, Metallography Principles and Practice, McGraw-Hill, Inc., 1984, p. 721.