Mo and some alloys - Chemical etching

Material Name: Mo and some alloys
Recipe No.: 10762
Primary Chemical Element in Material: Mo
Sample Type: Bulk
Uses: General microstructure
Etchant Name: None
Type (Macro/Micro): Micro
Etching Method: Chemical
Etchant (Electrolyte) Composition: Solution a: 10 g CuSO4 x 5H2O, 40 ml distilled water. Solution b: 20 ml NH4OH.
Procedure (Condition): Mix solution a, filter solution, add solution b. Immerse sample 30-50 s.
Note: For Mo and some alloys. Reveals grain structure. Millner and Sass.
Reference: Vander Voort, Metallography Principles and Practice, McGraw-Hill, Inc., 1984, p. 661.