Copper - Electrolytic polishing

Material Name: Copper
Recipe No.: 650
Primary Chemical Element in Material: Cu
Sample Type: Bulk
Uses: Polishing
Etchant Name: None
Type (Macro/Micro): Micro
Etching Method: Electrolytic polishing
Etchant (Electrolyte) Composition: 300 ml distilled water, 700 ml phosphoric acid.
Procedure (Condition): 5-15 min, 1.5-2 V dc, Cu cathode. After polishing, rinse in a 20% acueous solution of phosphoric acid.
Note: For all types of Cu and Cu Alloys, with exception of Sn bronzes.
Reference: Fred Hargreaves (Ret.), Personal Etchants Database 1960-1990, Analytical Services Bookham Technology, Caswell, Towcester, Northamptonshire NN8EQ, UK.